Master Class
A practical guide to welding thick aluminum using DC current and helium shielding gas.
Using DC- Current and Helium Gas to Weld Thick Aluminum
Gas tungsten arc welding (GTAW), also known as TIG welding, was a process developed in the early 1940s to weld materials such as magnesium and aluminum using an inert shielding gas such as helium. The TIG welding of aluminum is normally performed using AC polarity, and argon as the inert shielding gas because the positive side of the AC wave performs the oxide cleaning and the negative side performs the penetration to the base metal. If thicker sections need to be welded, however, it can be done using DC- polarity and pure helium gas. The DC- process delivers excellent weld penetration and profile while using less current than AC. It’s an option frequently used when the operator is using either a TIG machine that’s incapable of AC welding or a machine with a lower current output.
The use of helium as shielding gas creates hotter arc plasma than argon gas. This additional heat burns the oxidation off the aluminum during the welding, which eliminates the need for the alternating current.
Our demonstration can be found among the exclusive footage on the ARC website (arcmagazine.pub). It includes the welding of two sections of ¼-inch aluminum. Even though the helium gas burns the oxides off the aluminum as we weld, it’s important to manually clean the base metal with a stainless steel brush before starting in order to prepare the surface for the best possible weld.
We’re using a Lincoln Electric Aspect 375 TIG machine with a water cooler. The amperage is set at about 200 amps because more heat is focused on the base metal in DC- polarity than in AC. The helium is set at about 60 cubic feet per hour. A 4043 1/8-inch diameter electrode ensures the proper weld size for this thickness of aluminum material.
Careful monitoring of the weld is required to ensure you are maintaining proper weld size, which is typically about the same thickness as the base material. You also want to maintain consistent bead appearance without overheating the base metal due to aluminum’s high thermal conductivity. As you continue to weld, use your amptrol to slowly lower the amperage because the aluminum is becoming increasingly saturated with heat. Near the end of the weld, your amperage may be less than half of what you started with.
Notice that not all the oxides are completely burning off the surface, especially on the outer edges of the puddle. At the center of the puddle, however, the arc plasma created by the helium gas should eliminate the oxides and produce a desirable weld puddle.
If you examine the piece after the weld, you’ll probably see some oxide along the sides of the weld bead, but as far as the overall appearance, there should be complete fusion between the two base metals combined with the filler. As we welders like to say, it looks like a stack of dimes.
To summarize, alternating current is the preferred method of welding lightweight materials such as aluminum and magnesium, and current technology enables you to unbalance the AC waveform to favor the negative side of the AC wave and increase the level of heat and penetration to the base metal. If you don’t have a machine capable of high-amperage AC welding, you do have the option to weld aluminum with DC- polarity, but only if you use helium as the shielding gas. It will provide excellent penetration, acceptable cleaning of the oxides and a faster weld.
Master Class
A practical guide to welding thick aluminum using DC current and helium shielding gas.